Alloy Steel
  Steel name: Alloy Steel
  Diagram No.: 2887
  Type of diagram: TTE
  Chemical composition in weight %: 0.44% C, 1.64% Mn, 0.06% Si, 0.029% P, 0.022% S,
  1.84% Ni, 1.64% Cr, 0.40% Mo, 0.15% Cu.
  Note: Embrittlement diagram. Temper embrittlement. Austenitizing temperature: 900oC
  (1650oF). Grain szie: 6. Values given are average Charpy impact Test in ft-lb
  obtained on duplicate Test made at -60oF. All specimens were tempered at 1200oF to
  hardness of 230 Brinell, water quenched, held at the times and temperature indicated,
  and water quenched. See the diagrams No. 2886 and No. 2888.
  Source: W.S. Pellini, B.R. Queneau, "Developmnet of Temper Brittlness in Alloy Steel",
  Transactions of the ASM, Vol.39, ASM, 1947, p.139.