14 NC 11 Steel
  Steel name: 14 NC 11
  Diagram No.: 1725
  Type of diagram: TTT
  Mat. No. (Wr. Nr.) designation: 1.5732
  DIN designation: 14NiCr10
  AFNOR designation: 14 NC 11
  Chemical composition in weight %: 0.12% C, 0.51% Mn, 0.29% Si, 0.014% S, 0.013% P
  2.69% Ni, 0.70% Cr, 0.06% Mo, 0.18% Cu.
  Note: Alloy special structural steel. Austenitizing temperature: 850oC (1562oF) for
  30 min. Grain size: 9-11.
  Ac1: 730oC, Ac3: 800oC, Ms: 380oC.
  Source: Courbes de Transformation des Aciers de Fabrication Francaise, IRSID, Paris,
  France, 1974.